Properties |
Method |
Result |
Units |
|
Tensile Strength @ 73o
F |
D638-52T |
2000-4000 |
PSI |
Elongation @ 73o F |
|
200-400 |
% |
Young's Modulus @ 73o F |
Standard |
0.58
4.08 |
lbft/in2 X 105
kgf/cm2 X 105 |
Flexural Strength @ 73o
F |
ASTMD 790-61 |
did not break |
lbft/in2 |
Flexural Modulus @ 73o
F |
ASTMD 747-61T |
50000-90000 |
lbft/in2 |
Impact strength (Izod)@ 73o
F |
ASTMD 256-66 |
3.0 |
lbft/in2 |
Hardness durometer |
ASTMD 1706-59T |
D 50 - D 65 |
|
Compressive stress
@ 1% deformation @ 73o F
@ 1% offset @ 73o F |
ASTM 695-52T
ASTM 695-52T
|
600
1000 |
PSI
PSI |
Deformation under load (122o
F - 1000 PSI, 24 Hours) |
ASTM D621-59 |
2.4 |
% |
Deformation under load (122o
F - 2000 PSI, 24 Hours) |
ASTM D621-59 |
15 |
% |
|
|
|
Coefficient of linear thermal
Expansion per o F 73o F - 140 o F |
ASTMD 696-44 |
5.5X10-5 |
BTHU |
Thermal conductivity |
Cenco fitch Apparatus |
1.7 |
sq. ft/ o F/in |
Specific heat 0-212 o F
range |
- |
0.25 |
BTU/ib/o F |
Head deflection temp. @ 66 psi |
ASTMD 648-56 |
250 |
o F |
Heat resistance |
Standard |
500 |
o F |
|
Dielectric strength short time
0.080 in |
ASTMD 149-55T |
600 |
V/mil |
0.005-0.012 in |
" |
1000-2000 |
V /mil |
Volume resistivity |
ASTMD-257-57T |
108 |
ohm-cm |
Surface arc resistance |
ASTMD-495-56T |
>300 |
Sec. |
Dielectric constant @ 73o
F 50% RH |
ASTMD 150-54T |
21 |
|
Dissipation factor 60 to 2 X 109
cps |
ASTMD 150-59T |
0.0003 |
|
Power factor @ 73o F
50% RH |
ASTMD 150-54T |
<0.0003 |
|
|
Water Absorption 24 hours |
ASTMD 570-54T |
<0.01 |
% |
Flammability |
ASTMD 635-56T |
Non-flammable |
|
Specific gravity |
ASTMD 792-60T |
2.14 - 2.20 |
|
Resistance to weathering |
Standard |
Excellent |
|
Static kinetic coefficient of
friction against polish steel |
Various methods used |
0.05 to 0.08 |
|